{"id":2028,"date":"2026-01-20T17:36:04","date_gmt":"2026-01-20T22:36:04","guid":{"rendered":"https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/?post_type=chapter&#038;p=2028"},"modified":"2026-03-23T14:28:56","modified_gmt":"2026-03-23T18:28:56","slug":"the-importance-of-size-selection-in-size-reduction","status":"publish","type":"chapter","link":"https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/chapter\/the-importance-of-size-selection-in-size-reduction\/","title":{"raw":"3. The Importance of Size Selection in Size Reduction","rendered":"3. The Importance of Size Selection in Size Reduction"},"content":{"raw":"A size reduction circuit will typically involve more than one machine. The final material exiting a comminution circuit will have a specification for size, commonly to be less than some specified maximum. In many instances (not necessarily all), if the product is too big or too small it will not be adequately suited to the next step in the process, whether that is making a concentrate or extracting metals. But, size reduction machines typically produce quite a broad size distribution.\r\n\r\nWhile crushing machines produce a product with a set maximum size based on the machine discharge opening dimensions, grinding machines produce a distribution of sizes that depends on the length of time spent in the mill. If the ore charge is left in the mill long enough to ensure that the maximum size is less than some specified size, then much of the material will end up being too fine. This is called <span style=\"text-decoration: underline\">overgrinding<\/span>. But, if the charge is left in the mill for a short enough time to avoid forming too much fine material, then the largest particles will still be too big.\r\n\r\nThe solution is to leave the ore in the mill long enough so that a fraction of the ore is small enough, but not too small, then apply a size selection process to the discharged material. Material that is below a specified size passes on to the next step in the process. Material that is too large gets recycled to the mill for further grinding. We have already seen an application of size selection as applied to primary crushing. Oversize rocks that would clog a crusher can be screened out of the feed by use a \"grizzly\" screen. Screening is one method of selection or discrimination on the basis of size. Another very important method is the cyclone (or hydroclone where water is the fluid carrying particles rather than air). These select on the basis of differential movement of particles in fluids. There are numerous other size selection machines, but these two are the most common in mineral processing.\r\n\r\nWhen a mill product is size classified and oversize material is recycled back into the mill, this is called closed circuit size reduction. When there is no recycle of oversize back into a mill, this is called open circuit size reduction. Primary crushers are operated in open circuit fashion. Subsequent mills may be closed or open circuit. Some important features of each method are indicated below:\r\n\r\nOpen circuit:\r\n<ul>\r\n \t<li>Simplicity.<\/li>\r\n \t<li>Used if size classification is not practical.<\/li>\r\n \t<li>Used if product size range is not important.<\/li>\r\n \t<li>May be suitable for a rod mill which produces a somewhat narrower size distribution.<\/li>\r\n<\/ul>\r\nClosed circuit:\r\n<ul>\r\n \t<li>Greater control over the finished product size distribution.<\/li>\r\n \t<li>Increased mill capacity (time and energy are not wasted grinding the entire charge to less than a specified maximum size).<\/li>\r\n \t<li>Power requirements per tonne of finished ore are lowered (for the same reason as the preceding point).<\/li>\r\n \t<li>Less overgrinding and less production of extremely fine particles (smaller particles are removed).<\/li>\r\n \t<li>Costlier and more complex.<\/li>\r\n<\/ul>\r\n<h2>Screening<\/h2>\r\nScreens or sieves are surfaces with constant sized openings supported by a frame. Openings may be square, circular, rectangular, etc. Screens may be made of woven wires or perforated sheets. All particles that are smaller than the openings may, in principle, pass through. Particles larger than the openings may not pass through. Undersize may only contain particles less than the opening size. However, oversize that does not pass through may still contain undersized particles if not enough opportunity to contact the screen has been provided. Screens are typically vibrated up and down and side-to-side to maximize probability of contact between the ore particles and the mesh. They are also inclined to use gravity to force flow of the ore over the screen. A particle small enough to pass the screen might hit a wire and bounce off. And the smaller the particle size, the greater the probability that it will pass through. Thus the probability of a particle passing the screen is given by:\r\n\r\n\\[P = \\left(\\frac{D_A - d_0}{D_A + D_W}\\right)^2\\tag{2}\\]\r\n<blockquote>where D<sub>A<\/sub> = aperture width (square aperture)\r\nD<sub>W<\/sub> = screen wire thickness\r\nd<sub>0<\/sub> = diameter of a spherical particle<\/blockquote>\r\nA chart of the probability of passing through for a given number of attempts (number of times a particle contacts the screen) is shown in <a href=\"#table3.1\">Table 3.1<\/a>. The larger do is compared to DA the less likely it is to pass. The greater the number of contacts with the screen, the greater the chances of passing it. An inclined and vibrating screen increases the number of contacts. A problem with screens is \"blinding\". A particle somewhat too large to pass lodges in an opening and prevents other particles from passing through. This is illustrated in Figure 3.1 (below). Vertical vibration can help to loosen stuck particles. Optimum vertical stroke and horizontal frequency can vary with particle size. Larger particles require longer strokes and lower frequencies. Screens are classified according to their opening sizes and the number of wires per inch (mesh number). A 270 mesh sieve has 270 wires per inch. Obviously as the wires per inch increase the opening size decreases\r\nand the wire diameter decreases.\r\n\r\n<a id=\"table3.1\"><\/a>[table id=71 \/]\r\n\r\n[caption id=\"attachment_960\" align=\"aligncenter\" width=\"540\"]<img class=\"pb-hover-zoom wp-image-960 size-full\" src=\"https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F19_Screen_Blinding.png\" alt=\"Diagram with three evenly spaced circles and two shaded, irregular regions between them. The shaded areas, filled with dotted patterns, represent lodged particles that prevent smaller particles from passing through the screen.\" width=\"540\" height=\"226\" \/> Figure 3.1 - Illustration of blinding of a screen.[\/caption]\r\n\r\nThere are two general classifications, U.S. and Tyler. Table 3.2 indicates the mesh numbers and opening sizes. There are screens with larger openings too.\r\n\r\n[table id=72 \/]\r\n\r\n<em>*Very fine sieves are used in laboratories, but not in industrial screening as they are too fragile.<\/em>\r\n\r\nScreening cannot be used industrially below a minimum size since the screens become too fine and too fragile. Screening in air (dry screening) can be practiced down to about 5 mm. Wet screening is required for smaller particles wherein continuous water flow facilitates particle movement. For particles smaller than about 200-250 \u03bcm other types of size classifiers are commonly used. As particles size gets smaller the screen material itself occupies a greater fraction of the surface and throughput can become slow. Vibrating screens are a type of dynamic screen. There are other types of dynamic screens as well, e.g. drums. Screens may be static (unmoving) in some applications.\r\n\r\nAn interesting type of screen is the probability screen. Their apertures are substantially larger than desired particle size in the product. This type of screen relies on the fact that as particle size increases the probability of passing through decreases. If the frequency of encounters between the particles and the screen is kept low only the much smaller particles will pass through. For 10 attempts the probability of passing approaches 1 when do \u2248 0.1DA. Screening is complex. Estimation of the size of a screen needed should be determined by testing with actual ore to be processed.\r\n<h2>Classifiers<\/h2>\r\nTechnically classification refers to size selection on the basis of settling of solid particles under gravity in a fluid; air or water. Centrifugal forces may also be involved if particles are moving radially. All the forces involved are gravity, buoyancy, drag and centrifugal forces (where applicable). Depending on conditions such as viscosity, particle size and shape and particle velocity, laminar flow or turbulent flow of the fluid around the particle may occur. Terminal velocity is a key parameter for the settling rate. For laminar flow the terminal velocity is proportional to the square of the particle diameter. For turbulent flow it is related to the square root of diameter. There is less discrimination on the basis of size under turbulent flow conditions. Hence the possibility of separation of particles on the basis of settling rates depends critically on the flow regimes around the particles. Variations in density affect setting rates as well. This is minor for minerals with similar densities, but may be significant for minerals with much different densities (e.g. quartz: 2.65 g\/cm<sup>3<\/sup> and galena, PbS: 7.5 g\/cm<sup>3<\/sup>). It turns out that over the range 0.1 mm - 10 mm laminar flow, turbulent flow and combined regimes exist. This reduces selectivity. For &lt;100 \u03bcm particle sizes, the settling velocities become very low. This becomes impractical for industrial processes.* As particle size increases turbulent flow eventually dominates. Here since terminal velocity \u221d diameter1\/2, the settling rate is relatively less sensitive to particle size. Larger particles are generally best handled by screening.\r\n\r\n<em>*Fine particle size slurries can be effectively settled by adding flocculating agents that bind small particles into larger aggregates called flocs. Being tightly bound together, the more massive aggregate acts like a large particle and settles much more rapidly. This is suitable for solid-liquid separations, but it obviously defeats separation of particles on the basis of size.<\/em>\r\n\r\nFor particles of the same density the larger ones will fall fastest. For particles of the same size, the densest ones will fall fastest. Where differences in density are substantial a desired separation by classification is best suited to a somewhat coarser, more evenly sized ground ore. The product of a rod mill may be suitable here.\r\n\r\nFree settling involves a rather dilute [pb_glossary id=\"2074\"]slurry[\/pb_glossary], with a low concentration of particles. As particles fall in a more dense [pb_glossary id=\"2074\"]pulp[\/pb_glossary] they bump into each other. This slows settling and leads to what is called hindered settling. The system then behaves like a heavy liquid whose density is that of the pulp (water plus solids). Now resistance to fall is mainly due to turbulence. For spherical particles the terminal velocity is expressed as,\r\n\r\n\\[V_t = k \\left[ d(D_s - D_p) \\right]^{1\/2}\\tag{3}\\]\r\n<blockquote>k = proportionality constant (comprised of several physical terms).\r\nd = particle diameter.\r\nDs = particle density.\r\nDp = density of the pulp (weighted average density of water + solids).<\/blockquote>\r\nDs - Dp is the effective particle density. As pulp density* increases, the effective density of the solid particles (as Ds - Dp) decreases. Now large density differences between mineral particles becomes more important in hindered settling. Take the example of quartz and galena again. For a slurry with a density of 1.5 g\/mL (water has a density of 1 g\/mL) what size ratio of the two materials is required for both to have the same settling rate?\r\n\r\n\\[\\frac{v_{\\text{t galena}}}{v_{\\text{t quartz}}}= 1= k\\left[d_{\\text{quartz}}(2.65 - 1.5)\\right]^{1\/2}= k\\left[d_{\\ce{PbS}}(7.5 - 1.5)\\right]^{1\/2}\\tag{4}\\]\r\n\r\nThis yields\r\n\r\n\\[\\frac{d_{\\text{quartz}}}{d_{\\ce{PbS}}}= \\frac{7.5 - 1.5}{2.65 - 1.5}= 5.22\\tag{5}\\]\r\n\r\nSo a quartz particle 5.2 times the size of a galena particle will fall at the same rate. For free settling, the density of the fluid is the density of water. In this case,\r\n\r\n\\[\\frac{d_{\\text{quartz}}}{{d_{\\ce{PbS}}}} = 3.94\\tag{6}\\]\r\n\r\nHence the effect of density differences between minerals is amplified by hindering settling conditions. Free settling classifiers may be used when the separation is to be based predominantly on size and density differences are relatively small. Hindered settling classifiers are employed when the density differences between particles are to be exploited. Free settling requires a lot more water. Efficiency of settling is lower in hindered settling due to the increased viscosity of the fluid (slurry). Separation based on density differences is called sorting. This employs slurries with 40-70% solids by weight. Separation on the basis of particle size is called sizing. Slurries range from 3% solids for finer particles to 35% solids for coarse particles.\r\n\r\n<em>*Pulp density properly refers to the density (kg\/m<sup>3<\/sup>) of a slurry. The term is often used to refer to the % solids in a slurry. This is an unfortunate but common misuse of the term.<\/em>\r\n\r\nAn illustration of one type of classifier is shown in Figure 3.2 (below). These are cylindrical and have a conical bottom. They may be very large (on the order of up to 100 m) and have a large capital cost. Slurry feed enters near the centre and spreads over the surface. The overflow contains the undersize particles. The larger particles fall and are directed toward a centre outlet (underflow) by a slowly rotating rake. These utilize a horizontal current or flow. A number of these are may be used in series to achieve the desired separation. There are also other types of mechanical classifiers, for instance using a large screw in an inclined trough. Rotation of the screw lifts lighter particles up toward the overflow while gravity draws heavier particles down.\r\n\r\n[caption id=\"attachment_961\" align=\"aligncenter\" width=\"1180\"]<img class=\"pb-hover-zoom wp-image-961 size-full\" src=\"https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F20_Settler_Size_Classifier.png\" alt=\"Schematic diagram of a thickener used in mineral processing, showing a circular tank with central feed well introducing slurry. A rotating rake at the bottom moves solids toward the center for underflow discharge, while clarified liquid overflows at the edges.\" width=\"1180\" height=\"548\" \/> Figure 3.2 -\u00a0 Schematic diagram of a settler as a size classifier. The rake is turned very slowly to direct settled solids to the underflow.[\/caption]\r\n<h3>Cyclones and Hydroclones<\/h3>\r\nAlthough there are a great many types of size classifiers, many of these have been replaced by cyclones and hydroclones. They are the most prevalent size classifier in use in mineral processing. These machines use centrifugal force to increase the rate of particle segregation. Centrifugal forces of 10-4000 g may be employed, depending on the size of the machine. An illustration depicting how a cyclone (hydroclone) works is given in Figure 3.3 (below). Slurry enters the conical vessel tangentially at high rate. Heavier oversize particles stay against the wall and drop toward the bottom underflow. They follow a descending spiral path. The orbiting particles tend to be pushed toward the wall, but their movement is also impeded by drag forces. The smaller particles stay nearer the middle and tend to be drawn upwards by an inner vortex. The undersize particles exit through a central pipe at the top. This is called the vortex finder. It dips below the top of the cyclone and prevents the feed from simply exiting out the top. In a hydroclone an air core develops in the centre and the pressure in this region is quite low. In a hydroclone most of the liquid volume exits from the top. This drags the smaller particles with it. The flow pattern is complex. These machines are very efficient for separation of fine particle sizes. They find use in closed circuit grinding for separation of oversize and undersize particles, de-sliming (removal of very fine solids, called slimes), de-gritting (removal of coarse material) and thickening (which is partial removal of water from a slurry).\r\n\r\n[caption id=\"attachment_964\" align=\"aligncenter\" width=\"840\"]<img class=\"pb-hover-zoom wp-image-964 size-full\" src=\"https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F20_Hydroclone.png\" alt=\"Labeled diagram of a hydrocyclone showing tangential feed inlet, cylindrical-conical body, and internal flow paths. Outer vortex carries oversize particles downward to bottom outlet; inner vortex carries undersize particles upward through vortex finder at the top.\" width=\"840\" height=\"880\" \/> Figure 3.3 - Schematic illustration of the operation of a cyclone (hydroclone).[\/caption]\r\n\r\nHydroclones have replaced mechanical classifiers in modern grinding plants. Hydroclones are used for separations involving particles of between 5 and 150 \u03bcm. They are more efficient, especially in the fine particle range, they require less floor space, and the residence time is shorter. This may also have the added benefit of lessening the extent of oxidation of ore particles by air. Oxidation can be deleterious to downstream separation processes.\r\n\r\nThe efficiency of a hydroclone for separation of particles by size is represented by the partition curve. This is a plot of weight % of material reporting to the underflow versus size. A schematic example is shown in Figure 3.4 (below). For a perfectly efficient machine all the particles below a specified size would report to the overflow and all those above that size to the underflow. In reality, a curve is obtained. The size corresponding to the point where 50% of the mass goes to underflow and 50% to overflow is called the cutpoint or d<sub>50<\/sub>. Particles of this size have a 50-50 chance of reporting to either the overflow or the underflow. The steeper the slope in the vicinity of d<sub>50<\/sub>, the higher the efficiency.\r\n\r\nDesigners specify cyclones according to flow rates, with provision for adjustments to feed, overflow and underflow openings. The first parameter that needs to be known is the size at which the feed is to be split into oversize and undersize. This is the d<sub>50<\/sub>. The major factor in determining this is the cyclone diameter. A normal feed may contain up to 30% solids by weight. In closed circuit grinding operations up to 60% solids may be employed since the degree of separation\r\nrequired is not very fine. Capacities of 2000 - 2 \u00d7 10<sup>6<\/sup> m<sup>3<\/sup>\/h are possible.\r\n\r\n[caption id=\"attachment_965\" align=\"aligncenter\" width=\"1024\"]<img class=\"pb-hover-zoom wp-image-965 size-full\" src=\"https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F21_Partition_Curve_Hydroclone.png\" alt=\"Graph titled 'Partition curve for a hydroclone' showing particle size (\u00b5m) on the x-axis and weight percent to underflow on the y-axis. Includes a real sigmoidal curve and an ideal step curve, with d\u2085\u2080 marked at the 50% point\u2014indicating the particle size at which half report to underflow.\" width=\"1024\" height=\"634\" \/> Figure 3.4 - Partition curve for a cyclone (hydroclone).[\/caption]\r\n<h2>Size Reduction Circuits<\/h2>\r\nSize selection has already been seen to be an integral part of closed circuit size reduction. The preceding sections have described two of the most important size selection processes (screening and cyclones\/hydroclones). In addition to open circuit and closed circuit size reduction there is also single stage and two stage size reduction. For example, grinding can be done using a single type of mill (single stage grinding) or two types (two stage grinding). Some features of\r\nthese arrangements are indicated below:\r\n\r\nSingle stage:\r\n<ul>\r\n \t<li>Less equipment (lower capital and operating costs), simpler.<\/li>\r\n \t<li>Less space required.<\/li>\r\n<\/ul>\r\n2-stage:\r\n<ul>\r\n \t<li>Less overgrinding (greater flexibility and control).<\/li>\r\n \t<li>May allow for a simpler fine crushing plant (e.g. cone crushing; provides feed to the grinding plant).<\/li>\r\n \t<li>The capacity of an already existing single-stage grinding plant can be increased by addition of a second stage.<\/li>\r\n \t<li>Allows opportunity for recovery of desired ore material in between stages. Improves efficiency of throughput.<\/li>\r\n<\/ul>\r\nCrusher output particle size is not strongly dependent on input feed size. However, the output size from grinding mills is highly dependent on feed size because the output size depends critically on residence time in the mill. Hence screening of the final crushing plant product can help provide a more consistent feed to the grinding circuit. To get closely sized ground ore from a ball mill, AG mill and a SAG mill (where applicable; SAG mills may produce coarser material than an AG mill; AG mills are not common) closed circuit grinding is required.\r\n\r\nSome illustrative examples of size reduction flowsheets are presented in Figure 3.5 (below). There are numerous variations. In Figure 3.5 (A) (below) there is an illustration of a two stage grinding circuit. Another way to use the same equipment to potentially better effect is shown in Figure 3.5 (below). This too is a two-stage grinding circuit, but the cyclone\/hydroclone is placed between the rod mill and the ball mill, rather than after the ball mill as in Figure 3.5 (A) (below). The potential benefit of this arrangement is that output from the rod mill that is below the desired maximum size is removed as product without having to go through the ball mill. (Rod mill product may be more closely sized than ball mill product, but a size distribution is still produced.) This lessens overgrinding and allows greater throughput (or a smaller ball mill) since some rod mill product is removed ahead of the ball mill. The ball mill product is size classified through the same cyclone\/hydroclone.\r\n\r\nCriteria that influence design of size reduction circuits include:\r\n<ul>\r\n \t<li>Mill product specification (size range).<\/li>\r\n \t<li>Ore characteristics such as energy consumption for size reduction, feed size, variations in mineral hardness, etc.<\/li>\r\n \t<li>Optimization of energy efficiency (size reduction consumes a lot of energy).<\/li>\r\n \t<li>Minimization of capital cost.<\/li>\r\n \t<li>Production rate.<\/li>\r\n<\/ul>\r\n[caption id=\"attachment_966\" align=\"aligncenter\" width=\"1354\"]<img class=\"pb-hover-zoom wp-image-966 size-full\" src=\"https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F22_Size_Reduction_Circuits.png\" alt=\"Three ore processing flowcharts labeled A, B, and C. A: traditional three-stage crushing with jaw, secondary, and tertiary crushers, followed by screening and grinding in ball or rod mills. B: simplified flow with gyratory crusher feeding directly into AG mill. C: semi-autogenous process with gyratory crusher, SAG mill, and screening.\" width=\"1354\" height=\"1320\" \/> Figure 3.5 (A) - This is a multi-machine size reduction circuit and probably not all that common anymore. Crushing circuit product is passed over a screen. Oversize material is rejected and returned to the tertiary crusher (also a cone crusher).Undersize material is fed to the grinding circuit. The rod mill produces a suitably uniform feed to ball mill for final fine grinding. Product from the ball is fed to a cyclone; oversize is recycled to the ball mill. (B) Crushed ore from a gyratory (primary) crusher here is suitable as a feed to an AG mill in which it is ground. The product is classified and oversize is returned to the AG mill. (C) Crushed ore from a gyratory crusher is fed to a SAG mill. The SAG mill product is screened. Undersize is fed to a ball mill, the product of which is classified by a hydroclone. Oversize returns to the ball mill.[\/caption]\r\n\r\n<span style=\"background-color: #ccffff\">*add quiz*<\/span>","rendered":"<p>A size reduction circuit will typically involve more than one machine. The final material exiting a comminution circuit will have a specification for size, commonly to be less than some specified maximum. In many instances (not necessarily all), if the product is too big or too small it will not be adequately suited to the next step in the process, whether that is making a concentrate or extracting metals. But, size reduction machines typically produce quite a broad size distribution.<\/p>\n<p>While crushing machines produce a product with a set maximum size based on the machine discharge opening dimensions, grinding machines produce a distribution of sizes that depends on the length of time spent in the mill. If the ore charge is left in the mill long enough to ensure that the maximum size is less than some specified size, then much of the material will end up being too fine. This is called <span style=\"text-decoration: underline\">overgrinding<\/span>. But, if the charge is left in the mill for a short enough time to avoid forming too much fine material, then the largest particles will still be too big.<\/p>\n<p>The solution is to leave the ore in the mill long enough so that a fraction of the ore is small enough, but not too small, then apply a size selection process to the discharged material. Material that is below a specified size passes on to the next step in the process. Material that is too large gets recycled to the mill for further grinding. We have already seen an application of size selection as applied to primary crushing. Oversize rocks that would clog a crusher can be screened out of the feed by use a &#8220;grizzly&#8221; screen. Screening is one method of selection or discrimination on the basis of size. Another very important method is the cyclone (or hydroclone where water is the fluid carrying particles rather than air). These select on the basis of differential movement of particles in fluids. There are numerous other size selection machines, but these two are the most common in mineral processing.<\/p>\n<p>When a mill product is size classified and oversize material is recycled back into the mill, this is called closed circuit size reduction. When there is no recycle of oversize back into a mill, this is called open circuit size reduction. Primary crushers are operated in open circuit fashion. Subsequent mills may be closed or open circuit. Some important features of each method are indicated below:<\/p>\n<p>Open circuit:<\/p>\n<ul>\n<li>Simplicity.<\/li>\n<li>Used if size classification is not practical.<\/li>\n<li>Used if product size range is not important.<\/li>\n<li>May be suitable for a rod mill which produces a somewhat narrower size distribution.<\/li>\n<\/ul>\n<p>Closed circuit:<\/p>\n<ul>\n<li>Greater control over the finished product size distribution.<\/li>\n<li>Increased mill capacity (time and energy are not wasted grinding the entire charge to less than a specified maximum size).<\/li>\n<li>Power requirements per tonne of finished ore are lowered (for the same reason as the preceding point).<\/li>\n<li>Less overgrinding and less production of extremely fine particles (smaller particles are removed).<\/li>\n<li>Costlier and more complex.<\/li>\n<\/ul>\n<h2>Screening<\/h2>\n<p>Screens or sieves are surfaces with constant sized openings supported by a frame. Openings may be square, circular, rectangular, etc. Screens may be made of woven wires or perforated sheets. All particles that are smaller than the openings may, in principle, pass through. Particles larger than the openings may not pass through. Undersize may only contain particles less than the opening size. However, oversize that does not pass through may still contain undersized particles if not enough opportunity to contact the screen has been provided. Screens are typically vibrated up and down and side-to-side to maximize probability of contact between the ore particles and the mesh. They are also inclined to use gravity to force flow of the ore over the screen. A particle small enough to pass the screen might hit a wire and bounce off. And the smaller the particle size, the greater the probability that it will pass through. Thus the probability of a particle passing the screen is given by:<\/p>\n<p>\\[P = \\left(\\frac{D_A &#8211; d_0}{D_A + D_W}\\right)^2\\tag{2}\\]<\/p>\n<blockquote><p>where D<sub>A<\/sub> = aperture width (square aperture)<br \/>\nD<sub>W<\/sub> = screen wire thickness<br \/>\nd<sub>0<\/sub> = diameter of a spherical particle<\/p><\/blockquote>\n<p>A chart of the probability of passing through for a given number of attempts (number of times a particle contacts the screen) is shown in <a href=\"#table3.1\">Table 3.1<\/a>. The larger do is compared to DA the less likely it is to pass. The greater the number of contacts with the screen, the greater the chances of passing it. An inclined and vibrating screen increases the number of contacts. A problem with screens is &#8220;blinding&#8221;. A particle somewhat too large to pass lodges in an opening and prevents other particles from passing through. This is illustrated in Figure 3.1 (below). Vertical vibration can help to loosen stuck particles. Optimum vertical stroke and horizontal frequency can vary with particle size. Larger particles require longer strokes and lower frequencies. Screens are classified according to their opening sizes and the number of wires per inch (mesh number). A 270 mesh sieve has 270 wires per inch. Obviously as the wires per inch increase the opening size decreases<br \/>\nand the wire diameter decreases.<\/p>\n<p><a id=\"table3.1\"><\/a><\/p>\n<table id=\"tablepress-71\" class=\"tablepress tablepress-id-71\">\n<thead>\n<tr class=\"row-1\">\n<th colspan=\"4\" class=\"column-1\">Table 3.1 - Probability of a spherical particle passing a screen<\/th>\n<\/tr>\n<tr class=\"row-2\">\n<th rowspan=\"2\" class=\"column-1\">d<sub>0<\/sub>\/D<sub>A<\/sub><\/th>\n<th colspan=\"3\" class=\"column-2\">Probability of passing in %<\/th>\n<\/tr>\n<tr class=\"row-3\">\n<th class=\"column-2\">10 attempts<\/th>\n<th class=\"column-3\">100 attempts <\/th>\n<th class=\"column-4\">1000 attempts<\/th>\n<\/tr>\n<\/thead>\n<tbody class=\"row-striping row-hover\">\n<tr class=\"row-4\">\n<td class=\"column-1\">0.1<\/td>\n<td class=\"column-2\">97.5<\/td>\n<td class=\"column-3\">100<\/td>\n<td class=\"column-4\">100<\/td>\n<\/tr>\n<tr class=\"row-5\">\n<td class=\"column-1\">0.2<\/td>\n<td class=\"column-2\">94.8<\/td>\n<td class=\"column-3\">100<\/td>\n<td class=\"column-4\">100<\/td>\n<\/tr>\n<tr class=\"row-6\">\n<td class=\"column-1\">0.4<\/td>\n<td class=\"column-2\">83.9<\/td>\n<td class=\"column-3\">100<\/td>\n<td class=\"column-4\">100<\/td>\n<\/tr>\n<tr class=\"row-7\">\n<td class=\"column-1\">0.6<\/td>\n<td class=\"column-2\">57.0<\/td>\n<td class=\"column-3\">99.9<\/td>\n<td class=\"column-4\">100<\/td>\n<\/tr>\n<tr class=\"row-8\">\n<td class=\"column-1\">0.8<\/td>\n<td class=\"column-2\">20.8<\/td>\n<td class=\"column-3\">90.2<\/td>\n<td class=\"column-4\">100<\/td>\n<\/tr>\n<tr class=\"row-9\">\n<td class=\"column-1\">0.9<\/td>\n<td class=\"column-2\">6.3<\/td>\n<td class=\"column-3\">47.9<\/td>\n<td class=\"column-4\">99.8<\/td>\n<\/tr>\n<tr class=\"row-10\">\n<td class=\"column-1\">1<\/td>\n<td class=\"column-2\">0<\/td>\n<td class=\"column-3\">0<\/td>\n<td class=\"column-4\">0<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p><!-- #tablepress-71 from cache --><\/p>\n<figure id=\"attachment_960\" aria-describedby=\"caption-attachment-960\" style=\"width: 540px\" class=\"wp-caption aligncenter\"><img loading=\"lazy\" decoding=\"async\" class=\"pb-hover-zoom wp-image-960 size-full\" src=\"https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F19_Screen_Blinding.png\" alt=\"Diagram with three evenly spaced circles and two shaded, irregular regions between them. The shaded areas, filled with dotted patterns, represent lodged particles that prevent smaller particles from passing through the screen.\" width=\"540\" height=\"226\" srcset=\"https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F19_Screen_Blinding.png 540w, https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F19_Screen_Blinding-300x126.png 300w, https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F19_Screen_Blinding-65x27.png 65w, https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F19_Screen_Blinding-225x94.png 225w, https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F19_Screen_Blinding-350x146.png 350w\" sizes=\"auto, (max-width: 540px) 100vw, 540px\" \/><figcaption id=\"caption-attachment-960\" class=\"wp-caption-text\">Figure 3.1 &#8211; Illustration of blinding of a screen.<\/figcaption><\/figure>\n<p>There are two general classifications, U.S. and Tyler. Table 3.2 indicates the mesh numbers and opening sizes. There are screens with larger openings too.<\/p>\n<table id=\"tablepress-72\" class=\"tablepress tablepress-id-72\">\n<thead>\n<tr class=\"row-1\">\n<th colspan=\"6\" class=\"column-1\">Table 3.2 - Mesh numbers and opening sizes for wire sieves*.<\/th>\n<\/tr>\n<tr class=\"row-2\">\n<th colspan=\"2\" class=\"column-1\">Number\/mesh<\/th>\n<th rowspan=\"2\" class=\"column-3\">Opening mm<\/th>\n<th colspan=\"2\" class=\"column-4\">Number\/mesh<\/th>\n<th rowspan=\"2\" class=\"column-6\">Opening mm<\/th>\n<\/tr>\n<tr class=\"row-3\">\n<th class=\"column-1\">US<\/th>\n<th class=\"column-2\">Tyler<\/th>\n<th class=\"column-4\">US<\/th>\n<th class=\"column-5\">Tyler<\/th>\n<\/tr>\n<\/thead>\n<tbody class=\"row-striping row-hover\">\n<tr class=\"row-4\">\n<td class=\"column-1\">3.5<\/td>\n<td class=\"column-2\">3.5<\/td>\n<td class=\"column-3\">5.66<\/td>\n<td class=\"column-4\">60<\/td>\n<td class=\"column-5\">60<\/td>\n<td class=\"column-6\">250<\/td>\n<\/tr>\n<tr class=\"row-5\">\n<td class=\"column-1\">4<\/td>\n<td class=\"column-2\">4<\/td>\n<td class=\"column-3\">4.76<\/td>\n<td class=\"column-4\">70<\/td>\n<td class=\"column-5\">65<\/td>\n<td class=\"column-6\">210<\/td>\n<\/tr>\n<tr class=\"row-6\">\n<td class=\"column-1\">5<\/td>\n<td class=\"column-2\">5<\/td>\n<td class=\"column-3\">4.00<\/td>\n<td class=\"column-4\">80<\/td>\n<td class=\"column-5\">80<\/td>\n<td class=\"column-6\">177<\/td>\n<\/tr>\n<tr class=\"row-7\">\n<td class=\"column-1\">6<\/td>\n<td class=\"column-2\">6<\/td>\n<td class=\"column-3\">3.36<\/td>\n<td class=\"column-4\">100<\/td>\n<td class=\"column-5\">100<\/td>\n<td class=\"column-6\">149<\/td>\n<\/tr>\n<tr class=\"row-8\">\n<td class=\"column-1\">7<\/td>\n<td class=\"column-2\">7<\/td>\n<td class=\"column-3\">2.83<\/td>\n<td class=\"column-4\">120<\/td>\n<td class=\"column-5\">115<\/td>\n<td class=\"column-6\">125<\/td>\n<\/tr>\n<tr class=\"row-9\">\n<td class=\"column-1\">8<\/td>\n<td class=\"column-2\">8<\/td>\n<td class=\"column-3\">2.38<\/td>\n<td class=\"column-4\">140<\/td>\n<td class=\"column-5\">150<\/td>\n<td class=\"column-6\">105<\/td>\n<\/tr>\n<tr class=\"row-10\">\n<td class=\"column-1\">10<\/td>\n<td class=\"column-2\">9<\/td>\n<td class=\"column-3\">2.00<\/td>\n<td class=\"column-4\">170<\/td>\n<td class=\"column-5\">170<\/td>\n<td class=\"column-6\">88<\/td>\n<\/tr>\n<tr class=\"row-11\">\n<td class=\"column-1\">12<\/td>\n<td class=\"column-2\">10<\/td>\n<td class=\"column-3\">1.68<\/td>\n<td class=\"column-4\">200<\/td>\n<td class=\"column-5\">200<\/td>\n<td class=\"column-6\">74<\/td>\n<\/tr>\n<tr class=\"row-12\">\n<td class=\"column-1\">14<\/td>\n<td class=\"column-2\">12<\/td>\n<td class=\"column-3\">1.41<\/td>\n<td class=\"column-4\">250<\/td>\n<td class=\"column-5\">250<\/td>\n<td class=\"column-6\">63<\/td>\n<\/tr>\n<tr class=\"row-13\">\n<td class=\"column-1\">16<\/td>\n<td class=\"column-2\">14<\/td>\n<td class=\"column-3\">1.19<\/td>\n<td class=\"column-4\">270<\/td>\n<td class=\"column-5\">270<\/td>\n<td class=\"column-6\">53<\/td>\n<\/tr>\n<tr class=\"row-14\">\n<td class=\"column-1\">18<\/td>\n<td class=\"column-2\">16<\/td>\n<td class=\"column-3\">1.00<\/td>\n<td class=\"column-4\">325<\/td>\n<td class=\"column-5\">325<\/td>\n<td class=\"column-6\">44<\/td>\n<\/tr>\n<tr class=\"row-15\">\n<td class=\"column-1\">20<\/td>\n<td class=\"column-2\">18<\/td>\n<td class=\"column-3\">0.841<\/td>\n<td class=\"column-4\">400<\/td>\n<td class=\"column-5\">400<\/td>\n<td class=\"column-6\">37<\/td>\n<\/tr>\n<tr class=\"row-16\">\n<td class=\"column-1\">25<\/td>\n<td class=\"column-2\">24<\/td>\n<td class=\"column-3\">0.707 <\/td>\n<td class=\"column-4\"><\/td>\n<td class=\"column-5\">500<\/td>\n<td class=\"column-6\">30<\/td>\n<\/tr>\n<tr class=\"row-17\">\n<td class=\"column-1\">30<\/td>\n<td class=\"column-2\">28<\/td>\n<td class=\"column-3\">0.595<\/td>\n<td class=\"column-4\"><\/td>\n<td class=\"column-5\">600<\/td>\n<td class=\"column-6\">25<\/td>\n<\/tr>\n<tr class=\"row-18\">\n<td class=\"column-1\">35<\/td>\n<td class=\"column-2\">32<\/td>\n<td class=\"column-3\">0.500 <\/td>\n<td class=\"column-4\"><\/td>\n<td class=\"column-5\">750<\/td>\n<td class=\"column-6\">20<\/td>\n<\/tr>\n<tr class=\"row-19\">\n<td class=\"column-1\">40<\/td>\n<td class=\"column-2\">35<\/td>\n<td class=\"column-3\">0.420<\/td>\n<td class=\"column-4\"><\/td>\n<td class=\"column-5\">1000<\/td>\n<td class=\"column-6\">15<\/td>\n<\/tr>\n<tr class=\"row-20\">\n<td class=\"column-1\">45<\/td>\n<td class=\"column-2\">42<\/td>\n<td class=\"column-3\">0.354<\/td>\n<td class=\"column-4\"><\/td>\n<td class=\"column-5\">1500<\/td>\n<td class=\"column-6\">10<\/td>\n<\/tr>\n<tr class=\"row-21\">\n<td class=\"column-1\">50<\/td>\n<td class=\"column-2\">48<\/td>\n<td class=\"column-3\">0.297<\/td>\n<td class=\"column-4\"><\/td>\n<td class=\"column-5\"><\/td>\n<td class=\"column-6\"><\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p><!-- #tablepress-72 from cache --><\/p>\n<p><em>*Very fine sieves are used in laboratories, but not in industrial screening as they are too fragile.<\/em><\/p>\n<p>Screening cannot be used industrially below a minimum size since the screens become too fine and too fragile. Screening in air (dry screening) can be practiced down to about 5 mm. Wet screening is required for smaller particles wherein continuous water flow facilitates particle movement. For particles smaller than about 200-250 \u03bcm other types of size classifiers are commonly used. As particles size gets smaller the screen material itself occupies a greater fraction of the surface and throughput can become slow. Vibrating screens are a type of dynamic screen. There are other types of dynamic screens as well, e.g. drums. Screens may be static (unmoving) in some applications.<\/p>\n<p>An interesting type of screen is the probability screen. Their apertures are substantially larger than desired particle size in the product. This type of screen relies on the fact that as particle size increases the probability of passing through decreases. If the frequency of encounters between the particles and the screen is kept low only the much smaller particles will pass through. For 10 attempts the probability of passing approaches 1 when do \u2248 0.1DA. Screening is complex. Estimation of the size of a screen needed should be determined by testing with actual ore to be processed.<\/p>\n<h2>Classifiers<\/h2>\n<p>Technically classification refers to size selection on the basis of settling of solid particles under gravity in a fluid; air or water. Centrifugal forces may also be involved if particles are moving radially. All the forces involved are gravity, buoyancy, drag and centrifugal forces (where applicable). Depending on conditions such as viscosity, particle size and shape and particle velocity, laminar flow or turbulent flow of the fluid around the particle may occur. Terminal velocity is a key parameter for the settling rate. For laminar flow the terminal velocity is proportional to the square of the particle diameter. For turbulent flow it is related to the square root of diameter. There is less discrimination on the basis of size under turbulent flow conditions. Hence the possibility of separation of particles on the basis of settling rates depends critically on the flow regimes around the particles. Variations in density affect setting rates as well. This is minor for minerals with similar densities, but may be significant for minerals with much different densities (e.g. quartz: 2.65 g\/cm<sup>3<\/sup> and galena, PbS: 7.5 g\/cm<sup>3<\/sup>). It turns out that over the range 0.1 mm &#8211; 10 mm laminar flow, turbulent flow and combined regimes exist. This reduces selectivity. For &lt;100 \u03bcm particle sizes, the settling velocities become very low. This becomes impractical for industrial processes.* As particle size increases turbulent flow eventually dominates. Here since terminal velocity \u221d diameter1\/2, the settling rate is relatively less sensitive to particle size. Larger particles are generally best handled by screening.<\/p>\n<p><em>*Fine particle size slurries can be effectively settled by adding flocculating agents that bind small particles into larger aggregates called flocs. Being tightly bound together, the more massive aggregate acts like a large particle and settles much more rapidly. This is suitable for solid-liquid separations, but it obviously defeats separation of particles on the basis of size.<\/em><\/p>\n<p>For particles of the same density the larger ones will fall fastest. For particles of the same size, the densest ones will fall fastest. Where differences in density are substantial a desired separation by classification is best suited to a somewhat coarser, more evenly sized ground ore. The product of a rod mill may be suitable here.<\/p>\n<p>Free settling involves a rather dilute <a class=\"glossary-term\" aria-haspopup=\"dialog\" aria-describedby=\"definition\" href=\"#term_2028_2074\">slurry<\/a>, with a low concentration of particles. As particles fall in a more dense <a class=\"glossary-term\" aria-haspopup=\"dialog\" aria-describedby=\"definition\" href=\"#term_2028_2074\">pulp<\/a> they bump into each other. This slows settling and leads to what is called hindered settling. The system then behaves like a heavy liquid whose density is that of the pulp (water plus solids). Now resistance to fall is mainly due to turbulence. For spherical particles the terminal velocity is expressed as,<\/p>\n<p>\\[V_t = k \\left[ d(D_s &#8211; D_p) \\right]^{1\/2}\\tag{3}\\]<\/p>\n<blockquote><p>k = proportionality constant (comprised of several physical terms).<br \/>\nd = particle diameter.<br \/>\nDs = particle density.<br \/>\nDp = density of the pulp (weighted average density of water + solids).<\/p><\/blockquote>\n<p>Ds &#8211; Dp is the effective particle density. As pulp density* increases, the effective density of the solid particles (as Ds &#8211; Dp) decreases. Now large density differences between mineral particles becomes more important in hindered settling. Take the example of quartz and galena again. For a slurry with a density of 1.5 g\/mL (water has a density of 1 g\/mL) what size ratio of the two materials is required for both to have the same settling rate?<\/p>\n<p>\\[\\frac{v_{\\text{t galena}}}{v_{\\text{t quartz}}}= 1= k\\left[d_{\\text{quartz}}(2.65 &#8211; 1.5)\\right]^{1\/2}= k\\left[d_{\\ce{PbS}}(7.5 &#8211; 1.5)\\right]^{1\/2}\\tag{4}\\]<\/p>\n<p>This yields<\/p>\n<p>\\[\\frac{d_{\\text{quartz}}}{d_{\\ce{PbS}}}= \\frac{7.5 &#8211; 1.5}{2.65 &#8211; 1.5}= 5.22\\tag{5}\\]<\/p>\n<p>So a quartz particle 5.2 times the size of a galena particle will fall at the same rate. For free settling, the density of the fluid is the density of water. In this case,<\/p>\n<p>\\[\\frac{d_{\\text{quartz}}}{{d_{\\ce{PbS}}}} = 3.94\\tag{6}\\]<\/p>\n<p>Hence the effect of density differences between minerals is amplified by hindering settling conditions. Free settling classifiers may be used when the separation is to be based predominantly on size and density differences are relatively small. Hindered settling classifiers are employed when the density differences between particles are to be exploited. Free settling requires a lot more water. Efficiency of settling is lower in hindered settling due to the increased viscosity of the fluid (slurry). Separation based on density differences is called sorting. This employs slurries with 40-70% solids by weight. Separation on the basis of particle size is called sizing. Slurries range from 3% solids for finer particles to 35% solids for coarse particles.<\/p>\n<p><em>*Pulp density properly refers to the density (kg\/m<sup>3<\/sup>) of a slurry. The term is often used to refer to the % solids in a slurry. This is an unfortunate but common misuse of the term.<\/em><\/p>\n<p>An illustration of one type of classifier is shown in Figure 3.2 (below). These are cylindrical and have a conical bottom. They may be very large (on the order of up to 100 m) and have a large capital cost. Slurry feed enters near the centre and spreads over the surface. The overflow contains the undersize particles. The larger particles fall and are directed toward a centre outlet (underflow) by a slowly rotating rake. These utilize a horizontal current or flow. A number of these are may be used in series to achieve the desired separation. There are also other types of mechanical classifiers, for instance using a large screw in an inclined trough. Rotation of the screw lifts lighter particles up toward the overflow while gravity draws heavier particles down.<\/p>\n<figure id=\"attachment_961\" aria-describedby=\"caption-attachment-961\" style=\"width: 1180px\" class=\"wp-caption aligncenter\"><img loading=\"lazy\" decoding=\"async\" class=\"pb-hover-zoom wp-image-961 size-full\" src=\"https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F20_Settler_Size_Classifier.png\" alt=\"Schematic diagram of a thickener used in mineral processing, showing a circular tank with central feed well introducing slurry. A rotating rake at the bottom moves solids toward the center for underflow discharge, while clarified liquid overflows at the edges.\" width=\"1180\" height=\"548\" srcset=\"https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F20_Settler_Size_Classifier.png 1180w, https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F20_Settler_Size_Classifier-300x139.png 300w, https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F20_Settler_Size_Classifier-1024x476.png 1024w, https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F20_Settler_Size_Classifier-768x357.png 768w, https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F20_Settler_Size_Classifier-65x30.png 65w, https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F20_Settler_Size_Classifier-225x104.png 225w, https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F20_Settler_Size_Classifier-350x163.png 350w\" sizes=\"auto, (max-width: 1180px) 100vw, 1180px\" \/><figcaption id=\"caption-attachment-961\" class=\"wp-caption-text\">Figure 3.2 &#8211;\u00a0 Schematic diagram of a settler as a size classifier. The rake is turned very slowly to direct settled solids to the underflow.<\/figcaption><\/figure>\n<h3>Cyclones and Hydroclones<\/h3>\n<p>Although there are a great many types of size classifiers, many of these have been replaced by cyclones and hydroclones. They are the most prevalent size classifier in use in mineral processing. These machines use centrifugal force to increase the rate of particle segregation. Centrifugal forces of 10-4000 g may be employed, depending on the size of the machine. An illustration depicting how a cyclone (hydroclone) works is given in Figure 3.3 (below). Slurry enters the conical vessel tangentially at high rate. Heavier oversize particles stay against the wall and drop toward the bottom underflow. They follow a descending spiral path. The orbiting particles tend to be pushed toward the wall, but their movement is also impeded by drag forces. The smaller particles stay nearer the middle and tend to be drawn upwards by an inner vortex. The undersize particles exit through a central pipe at the top. This is called the vortex finder. It dips below the top of the cyclone and prevents the feed from simply exiting out the top. In a hydroclone an air core develops in the centre and the pressure in this region is quite low. In a hydroclone most of the liquid volume exits from the top. This drags the smaller particles with it. The flow pattern is complex. These machines are very efficient for separation of fine particle sizes. They find use in closed circuit grinding for separation of oversize and undersize particles, de-sliming (removal of very fine solids, called slimes), de-gritting (removal of coarse material) and thickening (which is partial removal of water from a slurry).<\/p>\n<figure id=\"attachment_964\" aria-describedby=\"caption-attachment-964\" style=\"width: 840px\" class=\"wp-caption aligncenter\"><img loading=\"lazy\" decoding=\"async\" class=\"pb-hover-zoom wp-image-964 size-full\" src=\"https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F20_Hydroclone.png\" alt=\"Labeled diagram of a hydrocyclone showing tangential feed inlet, cylindrical-conical body, and internal flow paths. Outer vortex carries oversize particles downward to bottom outlet; inner vortex carries undersize particles upward through vortex finder at the top.\" width=\"840\" height=\"880\" srcset=\"https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F20_Hydroclone.png 840w, https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F20_Hydroclone-286x300.png 286w, https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F20_Hydroclone-768x805.png 768w, https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F20_Hydroclone-65x68.png 65w, https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F20_Hydroclone-225x236.png 225w, https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F20_Hydroclone-350x367.png 350w\" sizes=\"auto, (max-width: 840px) 100vw, 840px\" \/><figcaption id=\"caption-attachment-964\" class=\"wp-caption-text\">Figure 3.3 &#8211; Schematic illustration of the operation of a cyclone (hydroclone).<\/figcaption><\/figure>\n<p>Hydroclones have replaced mechanical classifiers in modern grinding plants. Hydroclones are used for separations involving particles of between 5 and 150 \u03bcm. They are more efficient, especially in the fine particle range, they require less floor space, and the residence time is shorter. This may also have the added benefit of lessening the extent of oxidation of ore particles by air. Oxidation can be deleterious to downstream separation processes.<\/p>\n<p>The efficiency of a hydroclone for separation of particles by size is represented by the partition curve. This is a plot of weight % of material reporting to the underflow versus size. A schematic example is shown in Figure 3.4 (below). For a perfectly efficient machine all the particles below a specified size would report to the overflow and all those above that size to the underflow. In reality, a curve is obtained. The size corresponding to the point where 50% of the mass goes to underflow and 50% to overflow is called the cutpoint or d<sub>50<\/sub>. Particles of this size have a 50-50 chance of reporting to either the overflow or the underflow. The steeper the slope in the vicinity of d<sub>50<\/sub>, the higher the efficiency.<\/p>\n<p>Designers specify cyclones according to flow rates, with provision for adjustments to feed, overflow and underflow openings. The first parameter that needs to be known is the size at which the feed is to be split into oversize and undersize. This is the d<sub>50<\/sub>. The major factor in determining this is the cyclone diameter. A normal feed may contain up to 30% solids by weight. In closed circuit grinding operations up to 60% solids may be employed since the degree of separation<br \/>\nrequired is not very fine. Capacities of 2000 &#8211; 2 \u00d7 10<sup>6<\/sup> m<sup>3<\/sup>\/h are possible.<\/p>\n<figure id=\"attachment_965\" aria-describedby=\"caption-attachment-965\" style=\"width: 1024px\" class=\"wp-caption aligncenter\"><img loading=\"lazy\" decoding=\"async\" class=\"pb-hover-zoom wp-image-965 size-full\" src=\"https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F21_Partition_Curve_Hydroclone.png\" alt=\"Graph titled 'Partition curve for a hydroclone' showing particle size (\u00b5m) on the x-axis and weight percent to underflow on the y-axis. Includes a real sigmoidal curve and an ideal step curve, with d\u2085\u2080 marked at the 50% point\u2014indicating the particle size at which half report to underflow.\" width=\"1024\" height=\"634\" srcset=\"https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F21_Partition_Curve_Hydroclone.png 1024w, https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F21_Partition_Curve_Hydroclone-300x186.png 300w, https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F21_Partition_Curve_Hydroclone-768x476.png 768w, https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F21_Partition_Curve_Hydroclone-65x40.png 65w, https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F21_Partition_Curve_Hydroclone-225x139.png 225w, https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F21_Partition_Curve_Hydroclone-350x217.png 350w\" sizes=\"auto, (max-width: 1024px) 100vw, 1024px\" \/><figcaption id=\"caption-attachment-965\" class=\"wp-caption-text\">Figure 3.4 &#8211; Partition curve for a cyclone (hydroclone).<\/figcaption><\/figure>\n<h2>Size Reduction Circuits<\/h2>\n<p>Size selection has already been seen to be an integral part of closed circuit size reduction. The preceding sections have described two of the most important size selection processes (screening and cyclones\/hydroclones). In addition to open circuit and closed circuit size reduction there is also single stage and two stage size reduction. For example, grinding can be done using a single type of mill (single stage grinding) or two types (two stage grinding). Some features of<br \/>\nthese arrangements are indicated below:<\/p>\n<p>Single stage:<\/p>\n<ul>\n<li>Less equipment (lower capital and operating costs), simpler.<\/li>\n<li>Less space required.<\/li>\n<\/ul>\n<p>2-stage:<\/p>\n<ul>\n<li>Less overgrinding (greater flexibility and control).<\/li>\n<li>May allow for a simpler fine crushing plant (e.g. cone crushing; provides feed to the grinding plant).<\/li>\n<li>The capacity of an already existing single-stage grinding plant can be increased by addition of a second stage.<\/li>\n<li>Allows opportunity for recovery of desired ore material in between stages. Improves efficiency of throughput.<\/li>\n<\/ul>\n<p>Crusher output particle size is not strongly dependent on input feed size. However, the output size from grinding mills is highly dependent on feed size because the output size depends critically on residence time in the mill. Hence screening of the final crushing plant product can help provide a more consistent feed to the grinding circuit. To get closely sized ground ore from a ball mill, AG mill and a SAG mill (where applicable; SAG mills may produce coarser material than an AG mill; AG mills are not common) closed circuit grinding is required.<\/p>\n<p>Some illustrative examples of size reduction flowsheets are presented in Figure 3.5 (below). There are numerous variations. In Figure 3.5 (A) (below) there is an illustration of a two stage grinding circuit. Another way to use the same equipment to potentially better effect is shown in Figure 3.5 (below). This too is a two-stage grinding circuit, but the cyclone\/hydroclone is placed between the rod mill and the ball mill, rather than after the ball mill as in Figure 3.5 (A) (below). The potential benefit of this arrangement is that output from the rod mill that is below the desired maximum size is removed as product without having to go through the ball mill. (Rod mill product may be more closely sized than ball mill product, but a size distribution is still produced.) This lessens overgrinding and allows greater throughput (or a smaller ball mill) since some rod mill product is removed ahead of the ball mill. The ball mill product is size classified through the same cyclone\/hydroclone.<\/p>\n<p>Criteria that influence design of size reduction circuits include:<\/p>\n<ul>\n<li>Mill product specification (size range).<\/li>\n<li>Ore characteristics such as energy consumption for size reduction, feed size, variations in mineral hardness, etc.<\/li>\n<li>Optimization of energy efficiency (size reduction consumes a lot of energy).<\/li>\n<li>Minimization of capital cost.<\/li>\n<li>Production rate.<\/li>\n<\/ul>\n<figure id=\"attachment_966\" aria-describedby=\"caption-attachment-966\" style=\"width: 1354px\" class=\"wp-caption aligncenter\"><img loading=\"lazy\" decoding=\"async\" class=\"pb-hover-zoom wp-image-966 size-full\" src=\"https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F22_Size_Reduction_Circuits.png\" alt=\"Three ore processing flowcharts labeled A, B, and C. A: traditional three-stage crushing with jaw, secondary, and tertiary crushers, followed by screening and grinding in ball or rod mills. B: simplified flow with gyratory crusher feeding directly into AG mill. C: semi-autogenous process with gyratory crusher, SAG mill, and screening.\" width=\"1354\" height=\"1320\" srcset=\"https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F22_Size_Reduction_Circuits.png 1354w, https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F22_Size_Reduction_Circuits-300x292.png 300w, https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F22_Size_Reduction_Circuits-1024x998.png 1024w, https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F22_Size_Reduction_Circuits-768x749.png 768w, https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F22_Size_Reduction_Circuits-65x63.png 65w, https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F22_Size_Reduction_Circuits-225x219.png 225w, https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-content\/uploads\/sites\/1991\/2025\/10\/Ch2_F22_Size_Reduction_Circuits-350x341.png 350w\" sizes=\"auto, (max-width: 1354px) 100vw, 1354px\" \/><figcaption id=\"caption-attachment-966\" class=\"wp-caption-text\">Figure 3.5 (A) &#8211; This is a multi-machine size reduction circuit and probably not all that common anymore. Crushing circuit product is passed over a screen. Oversize material is rejected and returned to the tertiary crusher (also a cone crusher).Undersize material is fed to the grinding circuit. The rod mill produces a suitably uniform feed to ball mill for final fine grinding. Product from the ball is fed to a cyclone; oversize is recycled to the ball mill. (B) Crushed ore from a gyratory (primary) crusher here is suitable as a feed to an AG mill in which it is ground. The product is classified and oversize is returned to the AG mill. (C) Crushed ore from a gyratory crusher is fed to a SAG mill. The SAG mill product is screened. Undersize is fed to a ball mill, the product of which is classified by a hydroclone. Oversize returns to the ball mill.<\/figcaption><\/figure>\n<p><span style=\"background-color: #ccffff\">*add quiz*<\/span><\/p>\n<div class=\"media-attributions clear\" prefix:cc=\"http:\/\/creativecommons.org\/ns#\" prefix:dc=\"http:\/\/purl.org\/dc\/terms\/\"><h2>Media Attributions<\/h2><ul><li >Ch2_F18_Screen_Blinding  &copy;  B\u00e9 Wassink and Amir M. Dehkoda    is licensed under a  <a rel=\"license\" href=\"https:\/\/creativecommons.org\/licenses\/by-nc\/4.0\/\">CC BY-NC (Attribution NonCommercial)<\/a> license<\/li><li >Ch2_F19_Settler_Size_Classifier  &copy;  B\u00e9 Wassink and Amir M. Dehkoda    is licensed under a  <a rel=\"license\" href=\"https:\/\/creativecommons.org\/licenses\/by-nc\/4.0\/\">CC BY-NC (Attribution NonCommercial)<\/a> license<\/li><li >Ch2_F20_Hydroclone  &copy;  B\u00e9 Wassink and Amir M. Dehkoda    is licensed under a  <a rel=\"license\" href=\"https:\/\/creativecommons.org\/licenses\/by-nc\/4.0\/\">CC BY-NC (Attribution NonCommercial)<\/a> license<\/li><li >Ch2_F21_Partition_Curve_Hydroclone  &copy;  B\u00e9 Wassink and Amir M. Dehkoda    is licensed under a  <a rel=\"license\" href=\"https:\/\/creativecommons.org\/licenses\/by-nc\/4.0\/\">CC BY-NC (Attribution NonCommercial)<\/a> license<\/li><li >Ch2_F22_Size_Reduction_Circuits  &copy;  B\u00e9 Wassink and Amir M. Dehkoda    is licensed under a  <a rel=\"license\" href=\"https:\/\/creativecommons.org\/licenses\/by-nc\/4.0\/\">CC BY-NC (Attribution NonCommercial)<\/a> license<\/li><\/ul><\/div><div class=\"glossary\"><span class=\"screen-reader-text\" id=\"definition\">definition<\/span><template id=\"term_2028_2074\"><div class=\"glossary__definition\" role=\"dialog\" data-id=\"term_2028_2074\"><div tabindex=\"-1\"><p>A mixture of solution and solids. This is the state of an ore plus solution during and at the end of leaching. Complete dissolution does not occur.<\/p>\n<\/div><button><span aria-hidden=\"true\">&times;<\/span><span class=\"screen-reader-text\">Close definition<\/span><\/button><\/div><\/template><\/div>","protected":false},"author":2529,"menu_order":3,"template":"","meta":{"pb_show_title":"on","pb_short_title":"","pb_subtitle":"","pb_authors":[],"pb_section_license":""},"chapter-type":[],"contributor":[],"license":[],"class_list":["post-2028","chapter","type-chapter","status-publish","hentry"],"part":2014,"_links":{"self":[{"href":"https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-json\/pressbooks\/v2\/chapters\/2028","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-json\/pressbooks\/v2\/chapters"}],"about":[{"href":"https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-json\/wp\/v2\/types\/chapter"}],"author":[{"embeddable":true,"href":"https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-json\/wp\/v2\/users\/2529"}],"version-history":[{"count":15,"href":"https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-json\/pressbooks\/v2\/chapters\/2028\/revisions"}],"predecessor-version":[{"id":3843,"href":"https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-json\/pressbooks\/v2\/chapters\/2028\/revisions\/3843"}],"part":[{"href":"https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-json\/pressbooks\/v2\/parts\/2014"}],"metadata":[{"href":"https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-json\/pressbooks\/v2\/chapters\/2028\/metadata\/"}],"wp:attachment":[{"href":"https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-json\/wp\/v2\/media?parent=2028"}],"wp:term":[{"taxonomy":"chapter-type","embeddable":true,"href":"https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-json\/pressbooks\/v2\/chapter-type?post=2028"},{"taxonomy":"contributor","embeddable":true,"href":"https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-json\/wp\/v2\/contributor?post=2028"},{"taxonomy":"license","embeddable":true,"href":"https:\/\/pressbooks.bccampus.ca\/hydrometallurgy\/wp-json\/wp\/v2\/license?post=2028"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}